Imaginea produsului este cu titlul de referinta si poate sa nu corespunda cu produsul actual.
Diametre / Ambalaj
|
Diametre |
22.7 KG BAG |
|---|---|
| Flux | ED032990 |
DETALII
- Neutral submerged arc welding flux designed to meet the specific requirements of wind tower welding applications
- Recommended for use with Lincolnweld® L-61 electrode on both longitudinal and circumferential seam welds
- Capable of producing weld deposits with impact properties exceeding 27 J (20 ft·lbf) @ -62°C (-80°F)
- Smooth bead profile to achieve excellent toe angles, tie-in, and bead appearance on interior and exterior applications
Caracteristici
- Neutral submerged arc welding flux designed to meet the specific requirements of wind tower welding applications
- Recommended for use with Lincolnweld L-61 electrode on both longitudinal and circumferential seam welds
- Capable of producing weld deposits with impact properties exceeding 27 | (20 ft lbf) at --62 C (-80 F)
- Smooth bead profile to achieve excellent toe angles, tie-in, and bead appearance on interior and exterior applications
- Actual (Type 3.1) certificates for each lot of flux showing chemical composition, particle size and moisture level are available in the certificate center of lincolnwelectric.com
Informații despre service
S-ar putea să aveți nevoie și de
BEFORE USE, READ AND UNDERSTAND THE SAFETY DATA SHEET (SDS) FOR THIS PRODUCT AND SPECIFIC INFORMATION PRINTED ON THE PRODUCT CONTAINER. Pagina de căutare FDS
MECHANICAL PROPERTIES
| Wire | Classification | Postweld Heat Treatment |
Yield Strength @ 0.2% Offset
MPa (ksi) |
Tensile Strength
MPa (ksi) |
Elongation
% |
Charpy V-Notch
J (ft-lbs) @ -40°C (-40°F) |
Charpy V-Notch
J (ft-lbs) @ -50°C (-60°F) |
Charpy V-Notch
J (ft-lbs) @ -62°C (-80°F) |
|---|---|---|---|---|---|---|---|---|
| Lincolnweld® L-50® | F7A6-EM13K | As-welded | 500 (73) | 590 (86) | 29 | 89 (66) | ||
| Lincolnweld® L-56® | F9A6-EH11K-G | As-welded | 600 (87) | 700 (101) | 26 | 66 (49) | ||
| Lincolnweld® L-61® | F6P8-EM12K-H8 | 1 hour @ 620°C (1150°F) | 360 (52) | 460 (67) | 36 | 213 (157) | ||
| Lincolnweld® L-61® | F7A8-EM12K-H8 | As-welded | 410 (60) | 520 (75) | 31 | 88 (65) | ||
| Lincolnweld® L-70 | F8A4-EA1-A3-H8 | As-welded | 530 (77) | 610 (88) | 26 | 64 (47) | ||
| Lincolnweld® LA-71 | F7A6-EM14K-H8 | As-welded | 550 (80) | 630 (91) | 27 | 138 (102) | ||
| Lincolnweld® LA-75 | F7A4-ENi1K-G-H8 | As-welded | 500 (72) | 590 (86) | 29 | 144 (106) |
DEPOSIT COMPOSITION
| Wire | Classification | %C | %Cr | %Cu | %Mn | %Mo | %Ni | %P | %S | %Si | %Ti |
Diffusible Hydrogen
mL/100g Weld Metal |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Lincolnweld® L-50® | F7A6-EM13K | 0.05 | 0.08 | 2.12 | 0.015 | 0.004 | 0.45 | |||||
| Lincolnweld® L-56® | F9A6-EH11K-G | 0.05 | 0.05 | 0.08 | 2.47 | 0.01 | 0.03 | 0.014 | 0.003 | 0.76 | ||
| Lincolnweld® L-61® | F6P8-EM12K-H8 | 0.06 | 0.11 | 1.57 | 0.014 | 0.008 | 0.25 | 5 | ||||
| Lincolnweld® L-61® | F7A8-EM12K-H8 | 0.06 | 0.07 | 1.72 | 0.012 | 0.008 | 0.32 | 4 | ||||
| Lincolnweld® L-70 | F8A4-EA1-A3-H8 | 0.05 | 0.08 | 1.55 | 0.52 | 0.011 | 0.009 | 0.23 | 5 | |||
| Lincolnweld® LA-71 | F7A6-EM14K-H8 | 0.06 | 0.08 | 2.00 | 0.012 | 0.005 | 0.62 | 0.02 | 5 | |||
| Lincolnweld® LA-75 | F7A4-ENi1K-G-H8 | 0.06 | 0.03 | 0.10 | 1.93 | 0.00 | 0.86 | 0.012 | 0.006 | 0.46 | 5 |
FLUX COMPOSITION
| Classification | %Al2O3 | %CaF2 | %CaO | %FeO | %K2O | %MgO | %MnO | %Na2O | %SiO2 | %TiO2 | %ZrO2 |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Typical Result | 24 | 13 | 4 | 3 | 1 | 23 | 8 | 2 | 18 | 2 | 2 |