Master Class

Master Class | Friday, July 17, 2015 | United States



An in-depth technical guide explaining the science, procedures, and code requirements behind steel preheating for structural welding applications.

Master Class Department Header

PREHEATING STEEL:

Why, When and How

Preheating steel isn’t always necessary, as the majority of steel fabrication is done with materials that can be successfully welded without the need for additional preheat. That is because these steels have low hardenability due to their low carbon and alloy content. In addition, thinner sections often reduce or eliminate the need for preheat as the heat affected zones will experience slower cooling rates.

But there are times when we have to weld on thicker sections, or steel of higher strength, or alloy content that may require preheat. There are many codes that address the need for preheating the grades of steel applicable to that code. An example of a code would be the AWS D1.1 “Structural Welding Code for Steel.”

The primary reason for preheating is to slow the cooling rate of the weld and heat-affected base metal just underneath the weld. When we heat steel to a high temperature, which happens during welding, it transforms the steel’s basic structure and allows carbon atoms to move in between the iron atoms. If it cools slowly, the carbon has a chance to move back out, and the steel can return to a normal state. But if the steel cools too rapidly, the carbon can get trapped and the heated area under the weld will transform to a hard and brittle microstructure that can lead to cracking.

Preheating the base metal prior to welding allows the metal to cool down slowly. This is especially important as the material thickness increases, because thick, cold steel quenches the weld area faster. As the carbon or alloy content goes up, the hardening effect from rapid cooling is increased. The slower cooling rate also allows residual hydrogen more time to diffuse out of the weld and heat affected zone. Hydrogen contributes to cracking in welds and heat affected zones especially on thick restrained sections of steels with susceptible hard microstructures.

Preheating also can help reduce residual stresses and distortion, as well as help to ensure that weld metal mechanical properties, such as impact strength, are met.

In this demonstration, we will be working with a model of a structural steel connection similar to what might be found on a high-rise building, and we will assume that the AWS D1.1 code applies. In Table 3.2 of that code, the prequalified minimum preheat and interpass temperatures are specified based on the grade of steel, material thickness, and welding process used.

For demonstration purposes, we will say the flange on the column is 1 ¾ in. thick and made of an A 572 grade 50 steel, and the girder is made of an A 992 steel with a flange thickness of 1 in. For a field welding application, we would typically weld steels of this grade with the self-shielded flux-cored arc welding process.

image

Minimum Preheat Temperature

Per table 3.2, both A572 Gr 50 and A992 are listed as Category B steels. For FCAW welding, and for a steel more than 1 ½ in. thick through 2 ½ in. thick, a minimum 150° F preheat and interpass temperature is required. Clause 5.6 states that the preheat and interpass temperature should be checked just prior to initiating the arc for each pass.

Minimum Interpass Temperature

For large welds, more than one pass is required to achieve the required size. Interpass temperature is the temperature of the steel after the initial pass. The minimum interpass temperature is the same as the minimum preheat temperature. Minimum interpass temperature should be checked just prior to initiating each pass. Often the minimum interpass temperature can be maintained by the heat of continuous welding, but there are times when welding on thicker sections – or if welding is interrupted – that additional heat may need to be applied during welding to maintain minimum interpass temperature.

Where to Measure Preheat and Interpass Temperatures

The D1.1 code requires that minimum preheat and interpass temperature should be maintained for a distance at least equal to the distance of the thickest welded part (but not less than 3 in.) in all directions from the point of welding. Since the steel in our demonstration is less than 3 in. thick, we only have to measure preheat a minimum of 3 in. in all directions from the point of welding. If the steel were 5 in. thick, we would have to measure 5 in. in all directions from the point of welding.

I mark out an area at least 3 in. from the weld in all directions from the point of welding. This is the area that will be preheated – all the way through the thickness. If this were a 5 in. thick flange on a column, along with increasing the preheat to 225° F, we would also have to heat 5 in. in all directions from the point of welding.

Be sure to maintain minimum interpass temperature as welding progresses.

image

Pick Your Spot

Use soapstone to mark out the minimum area where preheat will occur, including the backside and bottom. The area doesn’t need to be 100% accurate as long as the minimum distance from the point of welding is measured. Use a temp stick to check the temperature of this area as the steel warms up.

As mentioned earlier, the steel will be welded with a low-hydrogen process. Typically, high-rise construction on a big building is welded with a semi-automatic process like shelf-shielded flux core.

The flat position T-joint, a bevel-grooved joint, would be welded with an E-70T-6 wire, such as an NR®-305, usually a 5/64 in. or 3/32 in. size. That would be the fastest way to weld these flat position welds. The vertical and overhead welds would be welded with a E- 71T-8 wire like Innershield® NR®-232 or NR®-233, usually with a 5/64 in. or 0.072 in. diameter. SMAW welding with low hydrogen electrodes such as Excalibur could also be used.

Measuring Preheat

There are several ways to measure preheat, such as infrared guns and thermal couples but temperature indicating crayons (i.e., temp sticks) are most commonly used because they are portable, cost effective and very accurate. It’s important to achieve the minimum temperature. Heating above the minimum is acceptable, but maximum interpass temperature must be avoided. Excessive interpass temperature could negatively affect mechanical properties such as notch toughness in both the weld and base metal.

image

The Process

Map out your territory with several marks to ensure applying and measuring heat the correct distance from the weld. Check your temperature on the opposite side that the heat is applied to assure heating through the entire thickness. Follow these steps for using the propane rosebud heater:

• Make sure you’re wearing your safety gear.
• Make sure all connections are tight.
• Turn on the propane tank valve.
• Open the oxygen tank valve all the way as it is a double seated valve.
• Set the fuel gas and oxygen pressure according to the tip manufacturer’s recommendation for the tip being used.
• Purge fuel gas and oxygen separately out of the line before lighting torch; 1 second for every 10 in. of hose.
• Partially open the fuel valve first and light the torch with a striker. Then open the torch oxygen valve to achieve a neutral flame. Continue to alternately adjust fuel gas and oxygen until the desired flame is attained.

When you first start preheating, the steel might appear to sweat. This is due to condensation resulting from the combustion of the oxy-fuel torch. The water is not coming from the steel itself.

As you warm up the steel, make sure the heat soaks into the web of the beam and all the way through the flange. You’ll soon start to see the temperature indicating crayon marks melt.

When the joint is heated to above the minimum interpass temperature, it’s ready for welding. When you achieve the required temperature, turn the torch off. If using alternate fuel such as oxy propane, turn the fuel gas valve at the torch off first to extinguish the flame, then turn the oxygen valve off at the torch. Turn off tanks, bleed off lines, and back regulator screw out when shutting torch down.

Remember to check between passes that you’re staying above the minimum interpass temperature of 150° F. In some cases, you’ll have to watch the upper interpass temperature, depending on what’s indicated by the code.

image
Master Class: Preheating Steel
image

Tools

Soapstone to mark area to be preheated

Temp stick to measure the temperature of the steel prior to welding

Oxy-propane torch (with striker)

Personal Protective Equipment

Heat-Resistant Welding Gloves
Safety Glasses
Welding Coat

image

PREHEAT SAFELY

We always want to make sure we’re working safely when welding and working with torches. Refer to ANSI Z49.1: “Safety in Welding, Cutting, and Allied Processes,” which includes heating.

Make sure to wear the proper safety gear, including flame-retardant clothing, gloves and proper safety glasses. Make sure your jeans or pants are not frayed.

For proper torch setup and application, refer to the manufacturer’s guidelines. Make sure to have the correct check valves on the torch, flash arresters back at the regulator, hoses in good condition, and regulators set and operating properly.