Ask the Experts

Ask the Experts | Friday, October 7, 2016 | United States



Expert guidance on selecting and using different TIG arc-starting methods for cleaner, more reliable welds.

Ask the Experts Department Header

I’m trying to select the right TIG machine. Can you help me understand the difference between Scratch, Touch and High-Frequency arc starting?

Jack Hunter, Union City, NJ

 

As your question suggests, there are three basic ways to initiate a TIG (gas tungsten arc welding) arc: scratch, touch and high frequency.

Scratch starting is usually used on material containing iron, like steel and stainless steel. To initiate the arc, use a sweeping motion to make contact with the metal (similar to lighting a match). It’s also important to note that the electrode is electrically hot at all times when scratch starting.


There are some drawbacks to scratch starting, though. The first is contamination at the beginning and end of the weld. There can be a tendency for the tungsten to stick to the base material (especially when the proper starting technique is not used), which can lead to tungsten inclusions. At the end of the weld, the arc is broken by pulling the torch back and rolling it to interrupt the welding circuit. When this is done, the gas coverage on the molten puddle is lost and oxidation occurs. Finally, there is no control over the amperage when scratch starting. If the machine is set to 120 amps, for example, it will run at 120 amps throughout the weld.

image
image

Touch starting (also known as lift starting) is not the same as scratch starting, but the terms are often mistakenly used interchangeably. Like scratch start, the tungsten is in contact with the metal — but that is where the similarities end. When touch starting, the tungsten is placed on the base material prior to activating the amptrol. Until the amptrol is activated the tungsten is not electrically hot and will not strike an arc.

When the pedal is pressed, lift the torch up to initiate the arc. Touch starting uses a lower open circuit voltage (OCV), meaning the equipment uses a very low voltage output until it realizes it has made continual contact with the work piece. Once lifted, the equipment will shift to a higher voltage output as the tungsten leaves the surface of the work piece. This preserves the tungsten points and creates little contamination. Because of the amptrol, users can control the amperage with touch starts.

High-frequency starting is a touchless method of arc starting. The tungsten should be held about 1/8th inch off the material. If equipped, make sure the power source is set to HF TIG or the toggle switch is set to high frequency. If a foot pedal is used, make sure to switch to remote so you can control the current. As you step on the foot amptrol or press the hand amptrol, the arc will jump the gap and initiate. There is little risk of contamination (tungsten inclusions) at the beginning of the weld, and there is no contact between the tungsten and base material. The gas flow (preflow) begins before the arc initiates and continues to flow once the amptrol is released and the arc is terminated. Post-flow will then continue, allowing the gas flow to protect the weld puddle.


This form of arc starting is very good for beginners, as it has the least amount of risk when it comes to tungsten contamination. Machines capable of high frequency are good for projects that require high-quality welds.

 

- Charles A. Lariche, Lincoln Electric Weld School Instructor

image
image

From the welding experts at
Lincoln Electric