Ask the Experts

Ask the Experts | Tuesday, September 26, 2017 | United States



Answers to common welding questions from industry professionals.

Ask the Experts Department Header

What is the easiest way to determine proper cup size and tungsten stick-out when welding either groove or fillet welds?
Geremy Massolin, Welland, Ontario

You always want to use the largest cup possible to ensure adequate gas coverage. Manufacturers make smaller cup sizes to fit in smaller welding spaces, but you generally want to use the largest cup size that you can fit in the space. For example, I wouldn’t try a fillet weld with a small number 4 cup if I can fit a 7 or 8 in the space. People tend to think the cup size determines the quality of a groove or fillet weld, but it doesn’t. In the end, it’s determined more by a combination of your tungsten size and your travel speed.

image

What is happening when the arc changes color if you touch your filler base or metal? What is the oxidizing point of your tungsten?
Jared Satuch, Fort Erie, Canada

If your tungsten is sticking out of the cup and the tip is turning purple, that means your post-flow of gas is insufficient. The tungsten is still too hot at the end of the weld, the argon gas quits, and oxide forms on the tungsten. So you want to add a few extra seconds of post-flow gas after you’ve finished welding to allow the tungsten to cool. This also prevents the oxidation. Consider purple a warning sign. The ideal color should be silver, or yellowish to silver. Any dark blue or purple means the tungsten is not getting enough gas to protect it, and it’s oxidizing too much.

image

What is the best way to clean oil-soaked aluminum castings before welding?
 John First, Gallatin, Missouri

Your best bet is to clean them in a mild alkaline – ideally in a dip tank, but a spray would also work. Other options include a solvent wipe with acetone, toluene, methyl ethyl ketone (MEK), trichlorobenzene (TCB) or chlorothane. Using a dechlorinated brake cleaner is another option. However, the mild alkaline is the most effective option if it’s available.

image

Here in Costa Rica, and generally in Latin America, MIG welders tend to use 100% CO2 with ER70S-6 wire, basically because it is cheaper. What are the advantages of using a CO2 / argon mix?
Enrique Calderón Ramírez, Paraiso, Cartago, Costa Rica

Changing gas in MIG welding is like knocking the flux off a stick electrode and putting a different flux on it. It changes the characteristics completely, depending on voltage, amperage and gas. You’re correct: 100% CO2 is cheaper than a CO2/argon mix, but 100% CO2 will give you a very volatile arc. It’s very choppy, and it creates a lot of spatter. You can get good penetration with it, but if you mix 75% argon and 25% CO2 – the standard short-arc mix – the argon calms the arc down and you get much less spatter, and a better bead appearance and better mechanical properties. And with a little bit of adjustment, you can get the same amount of penetration with the mixed gas. All you have to do is turn your wire feed speed up.

image

Can you explain what causes magnetism in the base material when welding, and how it can be prevented? When the arc starts to flutter and trail behind your direction of travel, it can really mess up the weld.
Will Painter, Raphine, Virginia

We’ll assume you’re referring to the magnetism that’s created by the arc during stick welding. The phenomenon is called arc blow. It won’t go away, but there are a few things you can do to make it more manageable:

  • The best way to minimize it is to switch to AC polarity, although that isn’t always an option.
  • Arc blow is generally not an issue when you’re welding at the middle of the plate, but when you’re at the end, the magnetism naturally bounces behind the electrode. However, if you attach a run-off tab – an extra piece of metal at the end of the plate – the magnetism will shift to the tab rather than bounce back.
  • The longer your arc, the more your voltage increases, and the more the magnetism will increase with it. When possible, try to weld in deep V groves to maintain a shorter arc length.
  • If you’re welding with a high amperage, you’re tendency toward magnetism is already higher, but changing your rod angle or torch angle should be helpful.
  • If you’re doing corner welds, start at the corner and weld outward. Welding toward the corner will just spit the magnetism outward and result in a sloppy weld.
  • Sometimes the position of your ground can affect the magnetism. Move your ground lead to another location – preferably the direction in which the magnetism is likely to jump, based on the direction of your weld.

You’ll never get rid of arc blow entirely. It’s a naturally occurring phenomenon. But if you can do some combination of these things, you’ll be able to manage it more easily.

From the welding experts at
Lincoln Electric