Master Class
purging stainless steel, stainless steel welding, TIG welding, weld quality, sugaring, welding techniques, corrosion resistance, pipe welding, welding education
Purging Stainless
Purging is the introduction of a gas on a weld of stainless steel or nickel alloy to remove atmosphere. The technique is typically used to improve not only the strength, integrity and reliability of a weld, but also the overall aesthetics.
When welding on stainless, we need to remove the atmosphere and replace it with a non-reactive gas to avoid the buildup of chromium oxide on the back side of the weld. This CrO₃ buildup is commonly referred to as “sugaring.” When it occurs, the facing side of the weld will look good, but the opposite side will have at least a tint or be covered in a black crust, with voids where the weld did not fuse together properly.
It’s important to avoid sugaring wherever possible, especially in specific industries where the tolerance for any contamination whatsoever is very low. In the food and pharmaceutical industries, for example, cracks in the processing system could potentially expose the product to bacterial contamination. The same holds true for the pipeline industry, where aqueous contamination can make its way into the crevices caused by sugaring. In a corrosive environment, this contamination can result in a leak of dangerous chemicals. Even stainless steel engine headers for automobiles and airplanes – parts that are subject to intense vibration – are prone to fracturing and malfunctioning if not properly purged.
And in any of these manufacturing scenarios, cracked welds can lead to contamination of materials inside the process, and also result in dangerous chemicals leaking into the environment where personnel are working.
Depending on what code you’re welding to, there will be a specification governing parts-per-million of oxygen on the backside of the weld. In most cases, the operator will attach a monitor to the pipe or tubing to measure that. Some codes, such as AWS 18.2, even have color charts for visual inspection of heat tint/sugaring.
Some extra equipment you will need will be a bottle of 100% argon, dual flow meter, an extra gas hose to run to your purge, a purge block, and painters tape or foil. In the video I will be doing a butt joint on 0.0625 stainless set up in a purge block. Argon gas will purge the bottom side while the torch provides the primary shielding from the top. If you are working with tubing or pipe, consider applying tape on one end with holes poked through for venting on that side while taping a tube to the opposite side to provide the argon.
When making your weld, make sure the purge hose is secure and does not fall out. Allow sufficient time for the gap to fully purge the piece.
If your purge was done properly, the back side of the piece should look clean, with a silver color throughout the weld. The welded surface should be free of cracks and crevices. If any of these factors appear to be amiss, your purge was probably not successful. You may be able to grind the base metal and retry. Otherwise, you’ll need to scrap the part and start over.